摘 要

四川某氧化铅锌矿,硫化铅锌矿含量较低,氧化铅易浮,氧化锌与脉石矿物嵌布较细,原矿铅的品位为3.62%、锌的品位为9.20%,采用磨矿细度为-325目占96.74%,铅锌顺序优先浮选工艺流程,闭路试验经过一粗一扫,三次精选优先浮选铅,一粗两扫,两次精选再浮选锌,可以得到铅精矿中Pb品位为51.01%,回收率达到85.74%,锌精矿中Zn品位为35.49%,回收率达到70.69%。

铅粗选部分:碳酸钠作为调整剂,经过实验确定,其最佳用量为150g/t;硫化钠作为活化剂,最佳用量为1500g/t;戊基黄药作为捕收剂,最佳用量为200g/t;2号油作为起泡剂,用量为20g/t;粗选时间为4min。铅精选部分:硫化钠最佳用量为100g/t;戊基黄药最佳用量为40g/t;精选时间为4min。

锌粗选部分:水玻璃作为矿泥分散剂,最佳用量为2000g/t;硫化钠最佳用量为25kg/t;十八胺作为捕收剂,最佳用量为650g/t;2号油最佳用量为100g/t;浮选浓度为24.7%,粗选时间为4min。锌精选中:水玻璃最佳用量为500g/t;硫化钠最佳用量为6kg/t;锌扫Ⅰ、Ⅱ浮选时间分别为5min。

关键词:氧化铅锌矿;浮选;铅锌分离;活化剂

Abstract

According to the mineral properties of Lead-Zinc oxide ore with low sufuration rate and better floatable lead oxide ore in Szechwan.The grade of lead is 3.62% and the grade of zinc is 9.20% in the raw ore.When the feeding grade of -0.054mm is 96.74% and adoptting the preferrential flotation process. One roughing-one scavengings-three cleanings can obtain lead concentrate and one roughing-two scavengings-two cleanings can obtain zinc concentrate in the closed-circuit test. The grade of lead concentrate is 51.01% and lead recovery is 85.75%.While the grade of zinc concentrate is 35.49% and zinc recovery is 70.69%.

In the lead rougher parts,sodium carbonate was used as adjusting agent.after the experiment to determine, optimum amount is 150g/t. sodium sulfide was used as the activating agent, optimal dosage is 1500g/t.amyl xanthate as collector,optimal dosage is 200g/t. No. 2 oil was used as the foaming agent, dosage is 20g/t.roughing time is 4min. Lead part of the selected, the optimum dosage of sodium sulfide is 100g/t. the best dosage of amyl xanthate is 40g/t.selection time is 4min.

In the zinc roughing parts, sodium silicate was used as slime dispersant, optimum amount is 2kg/t.the best dosage of sodium sulfide is 25kg/t.Octadecyl Amine was used as collectors, optimal dosage is 650g/t.the best dosage of No. 2 oil is 100g/t.flotation concentration was 24.7%. roughing time is 4min. In zinc concentration, sodium silicate of optimum dosage of 500g/t. the best dosage of sodium sulfide is 6kg/t.The time of zinc scan I and II flotation is about 5min.

Key Words:Lead-Zinc oxide ore;Flotation;The separation of Lead-Zinc;Activator

目录

摘 要 I

Abstract II

第一章 绪论 1

1.1资源概述 1

1.1.1铅的主要矿物及其资源概述 1

1.1.2锌的主要矿物及其资源概述 2

1.2氧化铅锌矿的主要矿物及其可浮性 3

1.3铅锌矿浮选药剂概述 3

1.3.1铅锌矿浮选调整剂 4

1.3.2铅锌矿浮选捕收剂 5

1.3.3铅锌矿浮选起泡剂 5

1.4课题主要研究内容与意义 6

1.4.1研究主要内容 6

1.4.2课题研究目的与意义 6

第二章 试样性质及研究方法 8

2.1原矿的制备 8

2.2试验设备及药剂 8

2.2.1试验设备 8

2.2.2试验药剂 8

2.2.3试验方法 9

第三章 氧化铅锌矿实验研究 10

3.1原矿的分析 10

3.1.1原矿多元素分析 10

3.1.2原矿主要化学成分分析 10

3.1.3化学物相分析 11

3.1.4小结 12

3.2磨矿细度试验 12

3.3铅浮选 15

3.3.1 铅粗选 15

3.3.2铅精选 18

3.4 锌浮选 20

3.4.1 锌粗选 20

3.4.2 锌精选 28

3.5 开路与闭路试验 30

3.5.1 开路试验 30

3.5.2 闭路试验 32

3.5.3 数质量流程图 33

第四章 结论 35

参考文献 36

致谢 38

第一章 绪论

1.1资源概述

1.1.1铅的主要矿物及其资源概述

1.1.1.1铅的主要性质

您需要先支付 50元 才能查看全部内容!立即支付